涂料缺陷 (Paint Defects)—— 干喷

企业   2025-01-18 15:00   江苏  
  ↑ 点击上方“涂料工业”关注我们

涂料工业:


涂料缺陷(Paint Defects)

七、干喷(Dry Spray)

1.描述(Description

漆膜表面粗糙和不均匀,颗粒没有足够的流动性,无法一起流动。这种涂层缺陷通常只有一小片范围。

Rough and uneven finish to the surface of the paint film where the particles are insufficiently fluid to flow together. This defect is normally limited to small areas.

图1 干喷示意图

2.可能原因(Probable Causes):

不正确的施工方法如喷枪与施工面的距离不适当。也与产品本身干燥过快和过高的施工温度有关。

Incorrect spray application i.e. gun distance. Also associated with fast drying products and too high an application temperature.

3.预防措施(Prevention):

使用正确的涂装设备和工艺。使用干燥较慢的溶剂或溶剂混合物。遵循推荐的施工程序。

Use correct coating application equipment and techniques. Use a slower drying solvent or solvent blend. Follow recommended application procedures.

4.修复方法(Repair):
等涂料干透后打磨,然后根据缺陷的大小,选择抛光或重新喷涂。重新喷涂需要喷砂去除任何松散的干喷,然后重新喷涂涂料或面漆。

Allow the paint to dry and then sand. After sanding, and depending on the magnitude of the defect, respraying or polishing will be necessary.Abrade and remove any loose dryspray and re-apply coating or topcoat.


下期预告:八、涂料缺陷 (paint defects)—— 鱼眼


AMPP工业涂装施工人员培训(ICA)课程4月下旬常州开班

(了解更多,请点击图片跳转)


编辑:朱致远、顾盛康

如需转载,请标注出处。

 专 业 合 作 伙 伴 
















涂料工业
“涂料工业”由全国涂料工业信息中心、中国化工学会涂料涂装专委会、钛白粉产业技术创新战略联盟、全国无机颜料信息站等机构联合推出。以专业视角,精选价值资讯,推送给涂料、颜料、涂装、腐蚀防护等行业。包含:资讯,数据,标准,观点,专访,会议,培训等
 最新文章